      Screen printing adhesion test methods

      Date:2016/6/3 8:56:55 Hits:6562
       

          (1) the thumb test

      Condition: the experimental samples more than 5 PCS

      Experimental procedure: take sample, with your thumb on the picture of the printing, with 3 + / - 0.5 0 KGF force polishing the try 15 times back and forth.

      Experimental determination: products printing patterns and poor gap/break/ink adhesion, otherwise is unqualified.

           (2) 75% alcohol test

      Requirements: 1, the experimental sample 5 PCS more than 2, 3, 75% alcohol 4 white cotton gauze, 1.5 + / - 1.5 0 KGF system is provided

         Experimental procedures: 1.5 KGF system tied at the bottom of white cotton gauze, dipped in 75% alcohol, and then with white cotton gauze back and forth between 30 on the printing design (about 15 SEC).

         Experimental determination: products printing design shall have no loss/break/ink adhesion and poor gap, allowing yan.1.5 + / - 0.5 0 KGF system, light color, but not fuzzy printing pattern should be clear, otherwise is unqualified.

      (3) the 95% alcohol test

      Requirements: 1, the experimental sample 5 PCS more than 2, 3, 95% alcohol 4 white cotton gauze, 1.5 + / - 1.5 0 KGF system is provided

      Experimental procedures: 1.5 KGF system tied at the bottom of white cotton gauze, dipped in 95% alcohol, and then use white cotton gauze back and forth between 30 on the printing design (about 15 SEC)

      Experimental determination: products printing design shall have no loss/break/ink adhesion and poor gap, allowing yan.1.5 + / - 0.5 0 KGF system, light color, but not fuzzy printing pattern should be clear, otherwise is unqualified.

      (4) 810 tape test conditions: 1, the test sample 5 PCS more than 2, 810 tape experimental programs: the 810 tape completely paste on the silk screen printing, and then to the direction of the 45 degree Angle quickly pull up the tape, measured three times in a row.

      Experimental determination: products printing design gap/break.

      (5) 3 m600 tape test

      Conditions: 1, the experimental sample 5 PCS more than 2, 2, 250 tape test program: 3 m600 tape completely paste in screen printing, at an Angle of 45 degrees direction quickly pull up the tape.Only need to test again.

      Experimental determination: products printing design gap/break.

      (6) 250 tape test

      Conditions: 1, the experimental sample 5 PCS more than 2, 250 tape experimental programs: the 250 tape completely paste in screen printing, at an Angle of 45 degrees direction quickly pull up the tape, three times in a row.

      Experimental determination: products printing design gap/break.

      (7) gasoline wipe the test

      Requirements: 1, the experimental sample 5 PCS more than 2, 3 white cotton gauze, gasoline mixture (gasoline: 75% alcohol = 1:1) 4, 1.5 + / - 1.5 0 KGF system is provided

      Experimental procedures: 1.5 KGF system tied at the bottom of white cotton gauze, dipped in gasoline mixture, back and forth between 30 on the printing design (about 15 SEC)

      Experimental determination: products printing design shall have no loss/gap/break/ink and poor adhesion, allowing partial light, color but not fuzzy printing pattern should be clear, otherwise is unqualified.

      (8) hexane brush try testing

      Requirements: 1, the experimental sample 5 PCS more than 2, white cotton gauze hexane 3, 4, 1.5 + / - 0.5 0 KGF system

      Experimental procedures: 1.5 KGF system tied at the bottom of white cotton gauze, dipped in hexane solution, back and forth between 30 on the printing design (about 15 SEC)

      The experiment to determine: ditto a judgement

      Remark:

      1, 2, 4 as the general standard,

      3, 6 for SEB commonly used standard,

      5 for JARDEN commonly used standard,

      7 as SOLAC common standard,

      8 for SUNBEAM Australia are commonly used

       

        Home About UsProduct Special promotions Case  News  Train  Message  Contact Us
      Links: Huai'an OLAT Pad PrintingScreenPrinting(Northern distribution)
      Copyright::OLAT PRINTING MACHINERY INDUSTRY CO.,LTD.
      ADD:No.9?Zhangji?Road?Economic?Development?Zone,?Kunshan,?Jiangsu?Province
      TEL:0512-57068888 FAX:0512-57068800
      国产精品男同志movies_久久天天躁狠狠躁夜夜AV浪潮_99久久免费国产香蕉麻豆_97久久天天综合色天天综合色hd
      <p id="p5tqn"><del id="p5tqn"><xmp id="p5tqn"></xmp></del></p>
      <acronym id="p5tqn"><strong id="p5tqn"></strong></acronym>
      <big id="p5tqn"></big>

      <table id="p5tqn"></table>